Introduction

Polymethyl methacrylate (PMMA) is the standard material for denture base due to its physical, mechanical, aesthetic and biocompatibility properties [1,2,3]. Different techniques can be used to manufacture dentures depending on the PMMA polymerization method (heat or cold-cured, microwaved or light-activated) and manufacturing processes such as compression or injection molding, 3D-milling or 3D-printing [1,2,3,4,5]. However, heat-cured PMMA resins remain the most widely used due to their low cost, their suitable properties and how easily they are fabricated or repaired [2].

Dentures are submitted to the buccal environment, masticatory forces and cleaning methods [1]. Hence, their longevity depends on the resin properties such as dimensional stability, surface hardness, flexural strength and elastic modulus [1, 6,7,8]. Dimensional stability ensures that a denture fits properly on the mucosa [6], while surface hardness is an indicator of potential resin degradation [8]. Flexural strength and elastic modulus are also essential mechanical properties to prevent dentures from fracturing under masticatory forces [6, 7].

However, the rough surface of heat-cured PMMA resin promotes adhesion and colonization by microorganisms such as C. albicans, mainly implicated in denture stomatitis [9,10,11]. This disease can lead to serious complications such as septicemia and even death, particularly in elderly or immunocompromised patients [9, 11, 12]. To prevent denture stomatitis, it is currently recommended to clean and disinfect dentures regularly, using disinfection solutions (e.g. sodium hypochlorite and chlorhexidine), denture cleansers (e.g. alkaline peroxide) and/or microwaves [6, 10, 12,13,14,15,16,17,18,19]. Despite their effectiveness to reduce Candida spp., the repeated and prolonged use of those treatments can lead to adverse effects compromising denture longevity such as resin whitening [10, 13, 20,21,22,23], distortion or shrinkage [6, 24,25,26,27,28], decreased surface hardness [17, 20, 29,30,31,32,33,34,35], and decreased flexural strength or elastic modulus [17, 22, 23, 32, 36, 37].

To avoid these adverse effects, non-thermal plasma could be used as an alternative technique. Plasma is an ionized gas consisting of electrons, ions, ultraviolet photons and neutral and reactive oxygen and nitrogen species, all of which could alter various microorganisms [38,39,40,41,42]. In previous studies, a technique based on non-thermal oxygen plasma generated in low-pressure (O2 NTP) conditions was developed, which inactivate various microorganisms, including C. albicans seeded on the surface of a heat-cured PMMA resin (ProBase® Hot, Ivoclar AG) [43,44,45,46,47]. A significant 6-log reduction in C. albicans viability was noted after a 120-minute treatment. Moreover, iterative O2 NTP treatment did not affect the visible aesthetics of ProBase® Hot resin [47]. Preserving other mechanical properties is nonetheless also essential to maintain the denture longevity.

The aim of this complementary study was therefore to assess the effects of O2 NTP treatments on some resin physical and mechanical properties. The null hypothesis was that O2 NTP treatments did not alter the dimensional stability, surface hardness, flexural strength or elastic modulus of the ProBase® Hot resin.

Materials and methods

Non-thermal O2 plasma treatment

The plasma prototype device (Aurora, Loos, France) and the process have been described by Ben Belgacem et al. [44]. Resin samples were placed inside a bag (Südpack® Medica, Ochsenhausen, Germany) which was sealed and then set on the radio-frequency (RF) polarization plate of the vacuum chamber (35 L). The bag was connected to the gas system. O2 gas was injected (1 sccm) through the first Tyvek® membrane of the bag when the low pressure reached 8 × 10-5 mbar. The excess gas was released through the second Tyvek® membrane of the bag into the vacuum chamber. Then, the discharge was induced by the RF polarization (100 W), and the plasma was densified inside the bag by the magnetic field (10 Gauss) for 120 min. Temperature did not exceed 40 °C during the entire treatment. At the end of the process, the vacuum chamber was returned to atmospheric pressure and the bag was disconnected.

Samples preparation

Samples were prepared from a heat-cured PMMA resin for denture base (ProBase® Hot 36 P-V, Ivoclar AG, Saint-Jorioz, France) using the heat-compression mold technique, according to the manufacturer’s instruction. Residual monomers were eliminated by storing the samples in distilled water for 24 h at room temperature. Shapes and dimensions of the resin samples were prepared and submitted to different treatments according to the different analyses (Table 1).

Table 1 Description of the groups according to the treatment applied

Full size table

Dimensional stability analysis

To analyze the dimensional stability, hemi cylinder-shaped (28.8 × 13.2 ×1.7 mm, n = 30) resin samples were produced and randomly divided among the treatment groups (C W, LP 1 W, P1 W and P6 W) (Fig. 1a and Table 1). A three-dimensional motorized measuring machine (Mistral, DEA, Hexagon Metrology, Villebon-sur-Yvette, France) with a 2 mm-diameter contact probe was used to record 64 points on the upper surface of each sample (Fig. 1b). This surface corresponded to the intaglio surface of the denture which is in contact with the palatal mucosa. The samples’ cylindricity was determined directly by the machine software (PC-DMIS® CAD + + 2010 MR3, Hexagon, Germany), by comparing them with a virtual hemi-cylindrical model. A support was fabricated to precisely position the samples while repeated measurements were recorded at a constant temperature of 20 °C (Fig. 1b). After immersion in distilled water to remove monomer residuals, all samples were dried and their initial cylindricity was recorded. Control samples (C W, n = 10) were submitted to six cycles alternating a 48-hour immersion in distilled water at 37 °C and a 20-min drying before a final measurement of the cylindricity. The samples of the LP1 W group (n = 10) were submitted to one previously-described cycle, then exposed to 120-min low pressure before measurement. The samples of the plasma group (n = 10) were submitted to six cycles alternating a 48-hour immersion in distilled water at 37 °C, a 20-min drying and a 120-min O2 NTP treatment. The cylindricity was recorded after the first (P1 W) and the sixth cycle (P6 W).

Fig. 1: Hemi cylinder-shaped resin sample.

a Sample dimensions; b Distribution of the 64 measuring points on the surface of the sample positioned on the support.

Surface hardness analysis

Ten bar-shaped samples (39 × 8 x 4 mm) were prepared for the Vickers hardness test. Microhardness was evaluated using a durometer (Wilson® VH1150, Buehler, Leinfelden-Echterdingen, Germany) with a Vickers indenter, under a 300 g (= 2,942 N) loading for 15 s. The hardness value before (C W) and after each treatment (LP1 W, P1 W and P6 W) was calculated from 10 measurement points spread along the samples (Table 1). Between each treatment, samples were stored in distilled water at 37 °C for 48 h and then dried.

Flexural strength and elastic modulus analyses

The flexural strength analysis was carried out according to ISO 20795-1 [48] and the elastic modulus was obtained from the previous results. Seven series of ten bar-shaped samples (64.0 ± 1.0 (L) x 10.0 ± 0.2 (h) x 3.3 ± 0.2 mm (b)) were produced and randomly divided according to the treatments (C D, C W, LP1 W, P1 W, LP6 W, P6 W, P6 D) (Table 1). The width (b) and the height (h) of all samples were recorded by digital caliper. After resin natural aging and treatments, the samples were stored in water at (37 ± 1) °C for (50 ± 2) h prior to testing. Then, the flexural strength of each sample was tested in a water bath at (37 ± 1) °C, using a three-point bending test on a MTS universal testing machine (DY-34; Adamel Lhomargy, Roissy-en-Brie, France). The distance between the center of the sample supports (l) was (50 ± 0.1) mm. The test was conducted until fracture under a crosshead speed of (5 ± 1) mm/min. The flexural strength (σ) (MPa) and the elastic modulus (E) (MPa) were calculated from the following formula:

$${{\rm{\sigma }}}=\frac{3{Fl}}{2b{h}^{2}}\,E=\frac{{F}_{1}{l}^{3}}{4b{h}^{3}d}$$

where F is the maximum load exerted (N), l the distance between the supports (mm), b the width, h the height of the sample (mm), F1 is the load at a point in the straight-line portion of the load/displacement curve (N), and d the deflection at load F1 (mm).

Scanning electron microscopy (SEM)

After the three-point bending test, two fractured resin’s samples from each group (C D, C W, LP1 W, P1 W, LP6 W, P6 W and P6 D) were prepared for SEM observations as previously described (Table 1) [47]. The samples were coated with gold/paladium on a Jeol Ion Sputter JFC-1100 and observed on a Jeol JSM-7900F Scanning Electron Microscope (PICT URCA Platform, Reims, France). Images were acquired from secondary electrons at a primary beam energy of 2 kV.

Statistical analysis

All statistical analyses were performed using GraphPad Prism version 8.0.2 for Windows, GraphPad Software. First, the Shapiro-Wilk test was used to assess normal or non-normal distribution of the datasets for each assay, and the Brown-Forsythe test was used to verify homogeneity of variances. Based on these results, appropriate statistical tests were selected to compare paired or independent groups. A p-value less than 0.05 was considered “statistically significant” (p < 0.05).

Concerning the dimensional stability, a multiple comparison was first performed using a one-way ANOVA to compare the initial cylindricity of all samples. Secondly, after each treatment, a pair-wise comparison was performed using a Student’s t-test to compare the samples’ dimension of the paired groups.

As for the surface hardness analysis, a non-parametric Wilcoxon t-test was used to compare paired groups. Regarding the analyses of the flexural strength and elastic modulus, a multiple comparison of the independent groups was performed using a one-way ANOVA followed by a Tukey’s post hoc test.

Results

Dimensional stability analysis

Table 2 summarizes the mean values of the resin ProBase® Hot samples’ cylindricity before and after each treatment (LP1 W, P1 W, P6 W) or after resin natural aging (C W). The values of the initial cylindricity of all samples were similar (from 28.551 ± 0.072 mm to 28.599 ± 0.071 mm, p = 0.306), showing homogeneity among them. Concerning the control group (C W), a significant difference of the dimension was noted after 3 weeks of resin natural aging, going from 28.551 ± 0.072 mm to 28.615 ± 0.068 mm (p < 0.001). A 120 min low pressure exposure (LP1 W) did not lead to any dimensional change (p = 0.758). After one (P1 W) or six O2 NTP treatments (P6 W), a slight significant change of the cylindricity was observed (p < 0.05).

Table 2 Mean values of cylindricity (mm) of the resin’s samples before and after each treatment (± SD)

Full size table

Surface hardness analysis

Table 3 summarizes the mean values of surface hardness of the ProBase® Hot resin samples, before (C W) and after each treatment (LP1 W, P1 W, P6 W). Before any treatment (C W), the mean surface hardness of the resin was 19.46 ± 0.89 (VHN). In comparison to this control value, only one O2 NTP treatment (P1 W) led to a significant change of the surface hardness (19.89 ± 0.63 (VHN), p < 0.05). This last treatment also showed a significantly higher hardness value in comparison to LP1 W and P6 W (19.36 ± 0.36 (VHN) and 19.33 ± 0.82 (VHN), respectively, p < 0.0001).

Table 3 Mean values of surface hardness (VHN) of the samples after each treatment and resin natural aging (± SD)

Full size table

Flexural strength and elastic modulus analyses

Figure 2 summarizes the mean values of the resin samples’ flexural strength (σ) and elastic modulus (E) after each treatment (LP1 W, P1 W, LP 6 W, P6 W, and P6 D) or after resin natural aging with or without rehydration (C W, C D).

Fig. 2: Three-point bending test results.

a Flexural strength and b elastic modulus of the samples after resin natural aging or after each treatment. The red lines represent the minimal σ and E thresholds defined by ISO 20795-1 norm. (*Significant differences between independent groups according to one-way ANOVA and post hoc Tukey’s test, p < 0.05). C W: untreated hydrated samples, C D: untreated dried samples, LP1 W: one 120-min low pressure exposure of hydrated samples, P1 W: one 120-min O2 NTP treatment of hydrated samples, LP6 W: six 120-min low-pressure exposures (between each treatment, the samples were immersed in distilled water at 37°C for 48 h), P6 W: six 120-min O2 NTP treatments (between each treatment, the samples were immersed in distilled water at 37 °C for 48 h), P6 D: six 120-min O2 NTP treatments (between each treatment, the samples were kept dried at 37 °C for 48 h).

ISO 20795-1 defines a minimal σ threshold (65 MPa) for Type 1 Class I PMMA denture base resin [48]. The ProBase® Hot resin met this norm with a mean σ of 75.5 ± 2.9 MPa (C D) (Fig. 2a). Six repeated hydrations of the resin (C W) at 37 °C did not alter the σ (74.7 ± 2.5 MPa) (p = 0.998). In the same way, no σ change was observed after one or six low pressure (LP1 W and LP6 W) or one O2 NTP (P1 W) exposures compared to the control (C W) (77.3 ± 3.3 MPa, 78.0 ± 3.7 MPa, and 77.6 ± 4.3 MPa, respectively, p > 0.05). After six repeated O2 NTP treatments, the hydrated resin samples (P6 W) showed a significantly lower σ under the threshold (47.6 ± 3.1 MPa, p < 0.001). On the opposite, the σ of the samples was similar to the control value (C D) when kept dried (P6 D) (78.4 ± 3.7 MPa, p = 0.567).

ISO 20795-1 defines a minimal E threshold (2000 MPa) for Type 1 Class I PMMA denture base resin [48]. The ProBase® Hot resin met this norm with a mean E of 2,322 ± 141 MPa (C D) (Fig. 2b). No significant difference was noted between groups C D, C W, LP1 W, P1 W and LP6 W (p > 0.05). After six repeated O2 NTP treatments, the hydrated resin samples (P6 W) showed a significant lower E (2,048 ± 75 MPa, p < 0.0001). However, this low value still met the E threshold. When kept dried (P6 D), the E of the samples was similar to the control value (C D) (2415 ± 150 MPa, p = 0.421).

SEM Analysis

Figure 3 shows the SEM images of the resin’s samples observed after the three-point bending test. All samples presented a rough surface characterized by porosities as well as lines resulting from the polishing process (Fig. 3a–e). No alteration was noted on the surface of hydrated samples exposed to low pressure (LP6 W) or one O2 NTP treatment (P1 W) (Fig. 3b and 3c, respectively) compared to the control (C W) (Fig. 3a). However, after six repeated O2 NTP treatments numerous cracks were observed on the surface of the samples only when they were hydrated (P6 W) and not when they were kept dry (P6 D) (Figs. 3d and e, respectively). The observation of the side crossed by fracture after the three-point bending test revealed an irregular surface of all resin’s samples (Fig. 3f–j). As for the cracks observed previously (Fig. 3d), they extended ~300 µm towards the center (Fig. 3i).

Fig. 3: SEM images of resin samples after natural resin aging and after different treatments.

The samples were observed after the three-point bending test at magnificence x60. a–e Upper sides of samples present a rough surface with porosities and lines due to polishing. f–j Sides crossed by fracture show an irregular resin’s surface. Only after P6 W treatment, the resin’s surface presents numerous fissures and cracks (d) (white arrows) that extend approximately 300 µm towards the material center (i). C W: untreated hydrated samples, LP6 W: six 120-min low-pressure exposures (between each treatment, the samples were immersed in distilled water at 37°C for 48 h), P1 W: one 120 min O2 NTP treatment of hydrated samples, P6 W: six 120 min O2 NTP treatments (between each treatment, the samples were immersed in distilled water at 37 °C for 48 h), P6 D: six 120 min O2 NTP treatments (between each treatment, the samples were kept dried at 37 °C for 48 h).

Discussion

The aim of this study was to evaluate the effects of O2 NTP treatment, generated in low pressure conditions, on the dimensional stability, surface hardness, flexural strength and elastic modulus of a heat-cured PMMA resin for denture base (ProBase® Hot, Ivoclar AG). The results showed that residual resin moisture only altered flexural strength and modulus of elasticity in the case of repeated plasma treatments. Consequently, the null hypothesis for repeated O2 NTP treatments can only be accepted if the resin is maintained under the controlled dry conditions described in this study.

The longevity of acrylic dentures depends on the preservation of the physical and mechanical properties of the resin [1, 6, 7]. However, the longevity can be undermined due to various factors such as the buccal environment, masticatory forces and cleaning methods [1]. To prevent C. albicans-associated denture stomatitis [9,10,11], different cleaning methods including disinfectants or denture cleansers and microwave radiations are commonly used or have been studied [6, 10, 12,13,14,15,16,17,18,19]. However, there is no consensus on a standard protocol of dentures’ disinfection due to their various adverse effects on the properties of heat-cured PMMA resins [6, 10, 13, 17, 19].

Non-thermal plasma processes have been studied as a new disinfection alternative to inactivate various microorganisms including C. albicans [38,39,40,41,42, 49, 50]. Within this field, a non-thermal O2 plasma generated under low-pressure conditions was developed, enabling the inactivation of microorganisms [43,44,45,46]. A previous study published in 2021 [47] demonstrated the efficacy of this non-thermal oxygen plasma (O2 NTP) treatment in reducing the viability of C. albicans seeded on ProBase® Hot resin (> 6 log) while preserving its aesthetics after repeated treatments. However, to ensure the longevity of dentures, the other resin properties must also be preserved, including dimensional stability, surface hardness, flexural strength and elastic modulus.

The dimensional stability of a resin is an essential parameter, as it ensures that a denture fits properly on the mucosa. Indeed, changes in denture dimensions can lead to injuries of the underlying tissues and induce bone resorption [6]. Over the last decade, the dimensional stability for denture base resin has been poorly investigated whatever the disinfection treatments used. Furthermore, there is no standardized protocol to assess this property, leading to various techniques using different devices (digital micrometer, digital caliper or microscope). Some authors have described that microwave radiations could lead to a shrinkage or a distortion of acrylic resins depending on different parameters: nature of the resin, power of microwaves, disinfection time, wet or dry conditions [6, 24,25,26,27,28]. In the present study, the results showed that O2 NTP treatment led to no or insignificant modification of the dimensional stability of the ProBase® Hot resin, as was found with some disinfection molecules (hypochlorite, povidone-iodine, or glutaraldehyde) [24, 51]. Indeed, exposure to low-pressure did not induce any dimensional change. But when exposed to one or six O2 NTP treatments, a slight significant change of the cylindricity was noted (−0.026 and +0.051 mm, respectively). However, this very slight variation was similar to the dimensional change due to the resin natural aging (+0.064 mm). Hence, these modifications would not have clinical incidence on the dentures fitting on the palatal mucosa.

The surface hardness of a denture base resin is an essential parameter to assess the behavior and degradation of the material over time [8]. In the literature, three techniques are usually described: Shore D [52, 53] Knoop [32, 34] and Vickers hardness, the latter being used most of the time [20, 29,30,31, 33, 35, 50]. It has been showed that longer or repeated chemical [17, 20, 29,30,31] and microwave treatments altered the surface hardness of heat-cured PMMA resins. In the current study, an increase of hardness was only noted after one O2 NTP exposure as in the study of Pan et al. [50] (Vertex Rapid Simplified PMMA resin; atmospheric plasma jet). However, this increase after O2 NTP treatment was considered insignificant as the hardness value (19.89 ± 0.63 (VHN)) was the same as the other groups’ (C W, LP1 W, P6 W) and as values found in the literature for heat-cured PMMA resins (from 16.18 ± 2.1 to 19.60 ± 0.60 (VHN)) [20, 31, 33, 35, 50]. Moreover, no modification was observed after six repeated treatments compared to the control. Hence, contrary to other disinfection techniques, long and repeated treatments using O2 NTP under low pressure condition did not significantly alter the surface hardness of the ProBase® Hot resin.

The ability of a denture to withstand masticatory forces depends, among other properties, on its flexural strength and elastic modulus [6, 7]. The flexural strength (σ) determines the maximum bending stress that can be applied to the denture until it fractures, while the elastic modulus (E) characterizes its stiffness and capacity to deform under bending stress. Concerning heat-cured PMMA resins, ISO 20795-1 or ADA No.12 specifications define a minimal σ threshold of 65 MPa and a minimal E threshold of 2000 MPa [48]. Chemical [17, 21, 23, 37, 54] and microwave [30, 33, 36] treatments did not alter or cause a decrease of the flexural strength and the elastic modulus of different PMMA resins below the minimum thresholds, except for longs or repeated treatments [17, 22, 32]. Regarding non-thermal atmospheric plasma jet (98% Ar and 2% O2), no significant change of Vertex Rapid Simplified resin was noted when a short-term treatment of 8.5 min (18 kV peak-to-peak voltage) was applied [50]. In the present study, low-pressure (10-5 mbar) did not alter the flexural strength and the elastic modulus after one or six exposures (LP1 W, LP6 W). But, when exposed to repeated O2 NTP treatments, a significant decrease of σ and E was observed below the minimal thresholds, only when the resin’s samples were kept in distilled water between each treatment (P6 W). This suggests that the presence of water was a decisive degradation factor when treatments were repeated.

Since few studies dealt with the degradation of heat-cured PMMA resin by non-thermal plasma, the focus was placed on the factors described in the literature that could explain why resin alters in the presence of moisture. A potential first factor could be the high rise in temperature that can induce chemical changes leading to depolymerization [55, 56]. Conversely, such deterioration cannot be attributed to thermal degradation, since the temperature inside the vacuum chamber does not exceed 40 °C. Another potential factor discussed in the literature claimed that water and UV radiations could result in the breaking of the polymer chains, generating radicals [55,56,57]. These radicals promote the bonding of oxygen molecules, leading to resin oxidation. These reactions cause internal stresses that result in the formation of cracks [57]. The plasma generated under the conditions used in this study was composed, among other things, of UV photons and reactive oxygen species [44]. If UV photons and reactive oxygen species alone appear insufficient to account for the observed degradation, residual moisture emerges as a critical factor. Indeed, cracks were observed only in samples rehydrated between successive exposures (P6 W). Although SEM imaging was performed post-mechanical testing—which precludes fully excluding a contribution from flexural stress—two observations support the role of moisture: the absence of cracks in dried samples (P6 D) and the significant reduction in flexural strength and elastic modulus in hydrated samples (P6 W). These findings support the hypothesis that residual moisture could play a key role in the degradation observed after repeated O2 NTP treatments, although further research is needed to establish a definitive causal link. This phenomenon could be explained by interactions between residual moisture and the elements generated by O2 plasma (such as reactive oxygen species and neutral molecules like O2). Indeed, water is absorbed by the resin’s surface and moisture can remain into porosities. With time, water molecules can penetrate between polymer molecular chains and act as plasticizers. As a result, they can increase the distance between these chains, thus decreasing the mechanical properties of resins, depending on their chemistry [6, 54, 58,59,60,61]. Moreover, Pan et al. [50] assumed that an oxidation of the resin’s surface by atmospheric plasma resulted in new chemical bonds in polymer molecular chains. Similarly, some authors described a degradation of the resins’ polymer matrix when exposed to denture cleansers (alkaline peroxide) diluted in water. Indeed, these chemical reactions lead to the production of hydrogen peroxide, oxygen molecules, and free oxygen radicals that are damaging for denture base materials when used for long-term treatments. Hence, preserving dentures from residual moisture is necessary to prevent any resin degradation during repeated O2 NTP treatments.

Considering the potential limitations of this study, further research would be helpful to clarify the mechanisms underlying the decrease in flexural properties observed when repeated O₂ NTP treatments are performed in the presence of residual moisture. Spectroscopic analyses could help identify surface chemical modifications induced by repeated O2 NTP exposure and rehydration. Future studies should also explore faster and measurable dehydration methods that optimize treatment duration while maintaining antifungal efficacy against C. albicans and preserving the resin’s properties. Additionally, the effects of O₂ NTP treatment should be compared to those of conventional disinfectants used for dentures in clinical conditions. Before conducting cytocompatibility studies, it will be necessary to determine whether similar results can be obtained using other working gases and to evaluate their effects on milled denture base resins with higher mechanical properties [4, 7, 8, 62, 63].

Conclusion

This study showed that O2 NTP treatment did not cause significant changes in the physical and mechanical properties of the heat-cured PMMA resin for denture base, when applied under controlled dehydration conditions. However, repeated exposure to O2 NTP in the presence of residual moisture significantly decreased its flexural strength and elastic modulus. This highlights the critical role of the resin’s hydration state during treatment. Therefore, O2 NTP appears to be a promising alternative approach to disinfect dentures, provided the resin’s hydration state is strictly controlled. These findings support further investigation into the use of O2 NTP for disinfecting dentures.

Data availability

The data supporting the results presented in the study are available from the generic space of “Recherche Data Gouv” multidisciplinary repository. (doi:10.57745/7P9YNU) URL: https://doi.org/10.57745/7P9YNU.

References

  1. Alqutaibi AY, Baik A, Almuzaini SA, Farghal AE, Alnazzawi AA, Borzangy S, et al. Polymeric denture base materials: a review. Polymers. 2023;15:3258.

    Article  PubMed  PubMed Central  CAS  Google Scholar 

  2. Le Bars P, Bandiaky ON, Le Guéhennec L, Clouet R, Kouadio AA. Different polymers for the base of removable dentures? Part I: a narrative review of mechanical and physical properties. Polymers. 2023;15:3495.

    Article  PubMed  PubMed Central  Google Scholar 

  3. Ivanova S, Tomova Z, Vlahova A, Stoeva IL, Vasileva E, Uzunova Y, et al. Contemporary use of polymers in dentistry: a narrative review. Polymers. 2026;18:138.

    Article  PubMed  PubMed Central  CAS  Google Scholar 

  4. de Oliveira Limírio J, Gomes J, Alves Rezende M, Lemos C, Rosa C, Pellizzer E. Mechanical properties of polymethyl methacrylate as a denture base: conventional versus CAD-CAM resin—a systematic review and meta-analysis of in vitro studies. J Prosthet Dent. 2022;128:1221–9.

    Article  PubMed  Google Scholar 

  5. Goodacre BJ. 3D printing of complete dentures: a narrative review. Int J Prosthodontics. 2024;37:S159–64.

    Article  Google Scholar 

  6. Klironomos T, Katsimpali A, Polyzois G. The effect of microwave disinfection on denture base polymers, liners and teeth: a basic overview. Acta Stomatol Croat. 2015;49:242–53.

    Article  PubMed  PubMed Central  Google Scholar 

  7. Aguirre BC, Chen JH, Kontogiorgos ED, Murchison DF, Nagy WW. Flexural strength of denture base acrylic resins processed by conventional and CAD-CAM methods. J Prosthet Dent. 2020;123:641–6.

    Article  PubMed  CAS  Google Scholar 

  8. Prpić V, Schauperl Z, Ćatić A, Dulčić N, Čimić S. Comparison of mechanical properties of 3D-printed, CAD/CAM, and conventional denture base materials. J Prosthodont. 2020;29:524–8.

    Article  PubMed  Google Scholar 

  9. Vila T, Sultan AS, Montelongo-Jauregui D, Jabra-Rizk MA. Oral candidiasis: a disease of opportunity. J Fungi. 2020;6:15.

    Article  CAS  Google Scholar 

  10. McReynolds DE, Moorthy A, Moneley JO, Jabra-Rizk MA, Sultan AS. Denture stomatitis—an interdisciplinary clinical review. J Prosthodont. 2023;32:560–70.

    Article  PubMed  Google Scholar 

  11. Perić M, Miličić B, Kuzmanović Pfićer J, Živković R, Arsić Arsenijević V. A systematic review of denture stomatitis: predisposing factors, clinical features, etiology, and global Candida spp. distribution. J Fungi. 2024;10:328.

    Article  Google Scholar 

  12. Yarborough A, Cooper L, Duqum I, Mendonça G, McGraw K, Stoner L. Evidence regarding the treatment of denture stomatitis. J Prosthodont. 2016;25:288–301.

    Article  PubMed  Google Scholar 

  13. Felton D, Cooper L, Duqum I, Minsley G, Guckes A, Haug S, et al. Evidence-based guidelines for the care and maintenance of complete dentures: a publication of the American College of Prosthodontists. J Prosthodont. 2011;20:S1–12.

    Article  PubMed  Google Scholar 

  14. Emami E, Kabawat M, Rompre PH, Feine JS. Linking evidence to treatment for denture stomatitis: a meta-analysis of randomized controlled trials. J Dent. 2014;42:99–106.

    Article  PubMed  CAS  Google Scholar 

  15. Ribeiro Rocha GDS, Neves Duarte T, de Oliveira Corrêa G, Nampo FK, de Paula Ramos S. Chemical cleaning methods for prostheses colonized by Candida spp.: a systematic review. J Prosthet Dent. 2020;124:653–8.

    Article  PubMed  Google Scholar 

  16. Ribeiro AB, Pizziolo PG, Clemente LM, Aguiar HC, Poker BC, Silva AAME, et al. Strategies for preventing and treating oral mucosal infections associated with removable dentures: a scoping review. Antibiotics. 2024;13:273.

    Article  PubMed  PubMed Central  CAS  Google Scholar 

  17. Zhang K, Zhang S, Shi Y, Zhang L, Fu B. Effects of disinfectants on physical properties of denture base resins: a systematic review and meta-analysis. J Prosthet Dent. 2024;131:841–58.

    Article  PubMed  CAS  Google Scholar 

  18. Polat Sagsoz N, Orhan F, Baris O, Sagsoz O. In vitro evaluation of plant antimicrobials against Candida albicans biofilm on denture base materials: a comparison with chemical denture cleansers. Polymers. 2025;17:2869.

    Article  PubMed  PubMed Central  CAS  Google Scholar 

  19. Nazer MW, Alzuwaihri AZ, Alakkad BA, Alamoudi MA, Alqurashi MH, Gharib AM, et al. A Comparison of the Efficacy of Non-chemical versus Chemical Cleansers against Candida Species on Removable Dental Prostheses: a Systematic Review. J Explor Res Pharmacol. 2026;11:e00041.

    Article  Google Scholar 

  20. Durkan R, Ayaz EA, Bagis B, Gurbuz A, Ozturk N, Korkmaz FM. Comparative effects of denture cleansers on physical properties of polyamide and polymethyl methacrylate base polymers. Dent Mater J. 2013;32:367–75.

    Article  PubMed  CAS  Google Scholar 

  21. Paranhos Hde F, Peracini A, Pisani MX, Oliveira Vde C, de Souza RF, de Silva-Lovato CH. Color stability, surface roughness and flexural strength of an acrylic resin submitted to simulated overnight immersion in denture cleansers. Braz Dent J. 2013;24:152–6.

    Article  PubMed  Google Scholar 

  22. Shah VR, Shah DN, Chauhan CJ, Doshi PJ, Kumar A. Evaluation of flexural strength and color stability of different denture base materials including flexible material after using different denture cleansers. J Indian Prosthodont Soc. 2015;15:367–73.

    Article  PubMed  PubMed Central  Google Scholar 

  23. Peracini A, Machado Andrade I, Oliveira VC, Macedo AP, Silva-Lovato CH, Oliveira Pagnano V, et al. Antimicrobial action and long-term effect of overnight denture cleansers. Am J Dent. 2017;30:101–8.

    PubMed  Google Scholar 

  24. Nirale RM, Thombre R, Kubasad G. Comparative evaluation of sodium hypochlorite and microwave disinfection on dimensional stability of denture bases. J Adv Prosthodont. 2012;4:24–9.

    Article  PubMed  PubMed Central  Google Scholar 

  25. Polychronakis N, Yannikakis S, Zissis A. The effect of repeated microwaving disinfection on the dimensional stability of acrylic dentures. Acta Stomatol Croat. 2014;48:279–84.

    Article  PubMed  PubMed Central  Google Scholar 

  26. Wagner DA, Pipko DJ. The effect of repeated microwave irradiation on the dimensional stability of a specific acrylic denture resin. J Prosthodont. 2015;24:25–31.

    Article  PubMed  Google Scholar 

  27. Polychronakis N, Polyzois G, Lagouvardos P, Andreopoulos A, Ngo HC. Long-term microwaving of denture base materials: effects on dimensional, color and translucency stability. J Appl Oral Sci. 2018;26:e20170536.

    Article  PubMed  PubMed Central  Google Scholar 

  28. da Costa RMB, Venante HS, Pordeus MD, Chappuis-Chocano AP, Neppelenbroek KH, Santiago Júnior JF, et al. Does microwave disinfection affect the dimensional stability of denture base acrylic resins? A systematic review. Gerodontology. 2022;39:339–47.

    Article  PubMed  Google Scholar 

  29. Porwal A, Khandelwal M, Punia V, Sharma V. Effect of denture cleansers on color stability, surface roughness, and hardness of different denture base resins. J Indian Prosthodont Soc. 2017;17:61–7.

    Article  PubMed  PubMed Central  Google Scholar 

  30. Kurt A, Erkose-Genc G, Uzun M, Sarı T, Isik-Ozkol G. The effect of cleaning solutions on a denture base material: elimination of Candida albicans and alteration of physical properties: effect of cleaning solutions on denture properties. J Prosthodont. 2018;27:577–83.

    Article  PubMed  Google Scholar 

  31. Ozyilmaz OY, Akin C. Effect of cleansers on denture base resins’ structural properties. J Appl Biomater Funct Mater. 2019;17:2280800019827797.

    PubMed  Google Scholar 

  32. Senna PM, Da Silva WJ, Faot F, Del Bel Cury AA. Microwave disinfection: cumulative effect of different power levels on physical properties of denture base resins. J Prosthodont. 2011;20:606–12.

    Article  PubMed  Google Scholar 

  33. Konchada J, Karthigeyan S, Ali SA, Amirisetty RV, Dani R. A. Effect of simulated microwave disinfection on the mechanical properties of three different types of denture base resins. J Clin Diagn Res. 2013;7:3051–3.

    PubMed  PubMed Central  Google Scholar 

  34. Capla M, Sardi JC, Pfeifer C, Consani RLX. Effect of different simulated microwave disinfection cycles on hardness, roughness and gloss of acrylic resins. Int J Dent Oral Sci. 2017;4:575–80.

    Google Scholar 

  35. Jaiswal P, Pande N, Banerjee R, Radke U. Effect of repeated microwave disinfection on the surface hardness of a heat-cured denture base resin: an in vitro study. Contemp Clin Dent. 2018;9:446–51.

    Article  PubMed  PubMed Central  CAS  Google Scholar 

  36. Hamouda IM, Ahmed SA. Effect of microwave disinfection on mechanical properties of denture base acrylic resin. J Mech Behav Biomed Mater. 2010;3:480–7.

    Article  PubMed  Google Scholar 

  37. Savabi O, Attar K, Nejatidanesh F, Goroohi H, Badrian H. Effect of different chemical disinfectants on the flexural strength of heat-polymerized acrylic resins. Eur J Prosthodont Restor Dent. 2013;21:105–8.

    PubMed  CAS  Google Scholar 

  38. Moisan M, Barbeau J, Moreau S, Pelletier J, Tabrizian M, Yahia LH. Low-temperature sterilization using gas plasmas: a review of the experiments and an analysis of the inactivation mechanisms. Int J Pharm. 2001;226:1–2.

    Article  PubMed  CAS  Google Scholar 

  39. Fiebrandt M, Lackmann JW, Stapelmann K. From patent to product? 50 years of low-pressure plasma sterilization. Plasma Process Polym. 2018;15:e1800139.

    Article  Google Scholar 

  40. Chen Z, Chen G, Obenchain R, Zhang R, Bai F, Fang T, et al. Cold atmospheric plasma delivery for biomedical applications. Mater Today. 2022;54:153–88.

    Article  CAS  Google Scholar 

  41. Kaushik N, Mitra S, Baek EJ, Nguyen LN, Bhartiya P, Kim JH, et al. The inactivation and destruction of viruses by reactive oxygen species generated through physical and cold atmospheric plasma techniques: current status and perspectives. J Adv Res. 2023;43:59–71.

    Article  PubMed  CAS  Google Scholar 

  42. Eslami H, Fakhrzadeh V, Nazari E, Katebi K, Alinejad M. Cold plasma treatment for Candida biofilm on resin base dentures: a systematic review. J Lasers Med Sci. 2025;16:e10 23.

    Article  PubMed  PubMed Central  Google Scholar 

  43. Ben Belgacem Z, Carré G, Boudifa M, Charpentier E, Cawe B, Gelle MP. Effectiveness of non-thermal O2-N2 plasma on P. aeruginosa multilayer biofilms cultured on hydroxyapatite. IRBM. 2016;37:68–74.

    Article  Google Scholar 

  44. Ben Belgacem Z, Carré G, Charpentier E, Le-Bras F, Maho T, Robert E, et al. Innovative non-thermal plasma disinfection process inside sealed bags: assessment of bactericidal and sporicidal effectiveness in regard to current sterilization norms. PLoS One. 2017;12:e0180183.

    Article  PubMed  PubMed Central  Google Scholar 

  45. Carré G, Charpentier E, Audonnet S, Terryn C, Boudifa M, Doliwa C, et al. Contribution of fluorescence techniques in determining the efficiency of the non-thermal plasma treatment. Front Microbiol. 2018;9:2171.

    Article  PubMed  PubMed Central  Google Scholar 

  46. Le Bras F, Carré G, Aguemon Y, Colin M, Gelle MP. Inactivation of enveloped bovine viral diarrhea virus and non-enveloped porcine Parvovirus using low-pressure non-thermal plasma. Life. 2021;11:1292.

    Article  PubMed  PubMed Central  Google Scholar 

  47. Maillet C, Odof S, Meuret M, Le Bras F, Velard F, Gelle MP. Non-Thermal O2 Plasma Efficacy on C. albicans and Its Effect on Denture Base Resin Color. Appl Sci. 2021;11:10367.

    Article  CAS  Google Scholar 

  48. ISO 20795-1: Dentistry—Base polymers—Part 1: Denture base polymers. International Organization for Standardization, Geneva, Switzerland. 2013. Available from: https://www.iso.org/standard/62277.html

  49. Matthes R, Jablonowski L, Koban I, Quade A, Hübner NO, Schlueter R, et al. In vitro treatment of Candida albicans biofilms on denture base material with volume dielectric barrier discharge plasma (VDBD) compared with common chemical antiseptics. Clin Oral Invest. 2015;19:2319–26.

    Article  Google Scholar 

  50. Pan H, Wang G, Pan J, Ye G, Sun K, Zhang J, et al. Cold plasma-induced surface modification of heat-polymerized acrylic resin and prevention of early adherence of Candida albicans. Dent Mater J. 2015;34:529–36.

    Article  PubMed  CAS  Google Scholar 

  51. Basavanna JM, Jujare RH, Varghese RK, Singh VD, Gaurav A. Effects of laboratory disinfecting agents on dimensional stability of three commercially available heat-cured denture acrylic resins in India: an in-vitro study. J Clin Diagn Res. 2016;10:ZC27–31.

    PubMed  PubMed Central  CAS  Google Scholar 

  52. Shihab RA. Impact of sorts disinfection and cleansing material on hardness of different types of denture base material. Tikrit J Dent Sci. 2017;5:135–42.

    Article  Google Scholar 

  53. Abdulwahhab SS. High-impact strength acrylic denture base material processed by autoclave. J Prosthodontic Res. 2013;57:288–93.

    Article  Google Scholar 

  54. Arruda CN, Sorgini DB, Oliveira Vde C, Macedo AP, Lovato CH, Paranhos Hde F. Effects of denture cleansers on heat-polymerized acrylic resin: a five-year-simulated period of use. Braz Dent J. 2015;26:404–8.

    Article  PubMed  Google Scholar 

  55. Yousif E, Haddad R. Photodegradation and photostabilization of polymers, especially polystyrene: review. SpringerPlus. 2013;2:398.

    Article  PubMed  PubMed Central  Google Scholar 

  56. Vohlídal J. Polymer degradation: a short review. Chem Teach Int. 2021;3:213–20.

    Article  Google Scholar 

  57. Sansul S, Yousif E, Ahmed DS, El-Hiti GA, Kariuki BM, Hashim H, et al. Pendant modification of poly(methyl methacrylate) to enhance its stability against photoirradiation. Polymers. 2023;15:2989.

    Article  PubMed  PubMed Central  CAS  Google Scholar 

  58. Bettencourt AF, Neves CB, de Almeida MS, Pinheiro LM, Oliveira SA, Lopes LP, et al. Biodegradation of acrylic based resins: a review. Dent Mater. 2010;26:e171–80.

    Article  PubMed  CAS  Google Scholar 

  59. Moghbelli E, Banyay R, Sue HJ. Effect of moisture exposure on scratch resistance of PMMA. Tribology Int. 2014;69:46–51.

    Article  CAS  Google Scholar 

  60. Lee HH, Lee JH, Yang TH, Kim YJ, Kim SC, Kim GR, et al. Evaluation of the flexural mechanical properties of various thermoplastic denture base polymers. Dent Mater J. 2018;37:950–6.

    Article  PubMed  CAS  Google Scholar 

  61. Geiger V, Mayinger F, Hoffmann M, Reymus M, Stawarczyk B. Fracture toughness, work of fracture, flexural strength and elastic modulus of 3D-printed denture base resins in two measurement environments after artificial aging. J Mech Behav Biomed Mater. 2024;150:106234.

    Article  PubMed  CAS  Google Scholar 

  62. Srinivasan M, Kamnoedboon P, McKenna G, Angst L, Schimmel M, Özcan M, et al. CAD-CAM removable complete dentures: a systematic review and meta-analysis of trueness of fit, biocompatibility, mechanical pro-perties, surface characteristics, color stability, time-cost analysis, clinical and patient-reported outcomes. J Dent. 2021;113:103777.

    Article  PubMed  CAS  Google Scholar 

  63. Fouda SM, Gad MM, Abualsaud R, Ellakany P, AlRumaih HS, Khan SQ, et al. Flexural properties and hardness of CAD-CAM denture base materials. J Prosthodont. 2023;32:318–24.

    Article  PubMed  Google Scholar 

Download references

Acknowledgements

The authors thank the “École d’ingénieurs en Sciences Industrielles et Numérique” (EiSINe) for providing their measuring instruments. Special thanks go to Walid Fekih Ahmed and Vincent Marquet (Université de Reims Champagne-Ardenne, ITHEMM, Reims, France) for their help in using the three-dimensional motorized measuring machine and the durometer. They also thank the “Laboratoire des Multimatériaux et Interfaces”, UMR CNRS 5615 (Univ Lyon, Université Claude Bernard Lyon 1, F-69622 Villeurbanne, France) in particular Pr. Brigitte Grosgogeat, for facilitating the flexural strength measurements. They thank URCATech-PICT platform (Université de Reims Champagne-Ardenne) for the access to imaging core facilities. Finally, the authors thank Marjorie Cantener (Université de Reims Champagne-Ardenne, UFR Odontologie, Reims, France) for her writing expertise and English language.

Funding

This research received no external funding.

Author information

Authors and Affiliations

  1. Université de Reims Champagne-Ardenne, BIOS, Reims, France

    Christina Maillet, Damien Bureau, Frédéric Velard, Sophie C. Gangloff & Marie-Paule Gelle

  2. Centre Hospitalier Universitaire de Reims, Pôle de Médecine Bucco-Dentaire, Reims, France

    Christina Maillet, Damien Bureau & Marie-Paule Gelle

  3. Université de Reims Champagne-Ardenne, UFR d’Odontologie, Reims, France

    Christina Maillet, Damien Bureau & Marie-Paule Gelle

  4. Université de Reims Champagne-Ardenne, ITHEMM, Reims, France

    Yessine Toumi

  5. Univ Lyon, Université Claude Bernard Lyon 1, UMR CNRS 5615, Laboratoire des Multimatériaux et Interfaces, Villeurbanne, France

    Hazem Abouelleil

  6. Univ Lyon, Faculté d’Odontologie, Lyon, France

    Hazem Abouelleil

  7. Université de Reims Champagne-Ardenne, UFR de Pharmacie, Reims, France

    Sophie C. Gangloff

Authors

  1. Christina Maillet
  2. Damien Bureau
  3. Yessine Toumi
  4. Frédéric Velard
  5. Hazem Abouelleil
  6. Sophie C. Gangloff
  7. Marie-Paule Gelle

Contributions

CM: Conceptualization, Methodology, Investigation, Writing-Original Draft, Visualization. DB: Methodology, Investigation, Writing-Original Draft. YT: Methodology, Investigation. FV: Investigation. HA: Methodology, Investigation. SCG: Visualization, Writing-Original Draft. M-PG: Conceptualization, Methodology, Writing-Original Draft, Visualization, Supervision, Project administration. All authors read and approved the final version of the manuscript.

Corresponding author

Correspondence to Christina Maillet.

Ethics declarations

Competing interests

The authors declare no competing interests.

Additional information

Publisher’s note Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Rights and permissions

Open Access This article is licensed under a Creative Commons Attribution-NonCommercial-NoDerivatives 4.0 International License, which permits any non-commercial use, sharing, distribution and reproduction in any medium or format, as long as you give appropriate credit to the original author(s) and the source, provide a link to the Creative Commons licence, and indicate if you modified the licensed material. You do not have permission under this licence to share adapted material derived from this article or parts of it. The images or other third party material in this article are included in the article’s Creative Commons licence, unless indicated otherwise in a credit line to the material. If material is not included in the article’s Creative Commons licence and your intended use is not permitted by statutory regulation or exceeds the permitted use, you will need to obtain permission directly from the copyright holder. To view a copy of this licence, visit http://creativecommons.org/licenses/by-nc-nd/4.0/.

Reprints and permissions

About this article

Check for updates. Verify currency and authenticity via CrossMark

Cite this article

Maillet, C., Bureau, D., Toumi, Y. et al. Effects of low-pressure non-thermal oxygen plasma treatments on mechanical properties of a PMMA resin for denture base. BDJ Open 12, 106 (2026). https://doi.org/10.1038/s41405-026-00499-w

Download citation

  • Received: 17 July 2026

  • Revised: 15 September 2026

  • Accepted: 16 September 2026

  • Published: 18 November 2026

  • Version of record: 18 November 2026

  • DOI: https://doi.org/10.1038/s41405-026-00499-w

来源:Nature 健康护理主题 · nature.com