Introduction

Dentin biomodification is a therapeutic approach based on biomimetic principles that aims to reinforce and stabilize the collagen matrix through chemical modulation of dentin collagen [1]. This strategy has been investigated to improve the stability of the adhesive interface by reinforcing the dentin collagen matrix and enhancing resin–dentin bonding [1,2,3]. Natural bioactive compounds, particularly polyphenols and flavonoids, have attracted interest as dentin biomodifiers because of their potential to interact with collagen and modulate enzymes involved in extracellular matrix degradation [4, 5].

Among natural dentin biomodifiers, epigallocatechin-3-gallate (EGCG) and proanthocyanidins (PAs) have demonstrated the ability to interact with and stabilize the collagen matrix [1, 6,7,8]. However, the potential clinical application of natural biomodifying agents may be limited by factors such as chemical instability and substrate discoloration [1, 5, 6, 9]. These limitations are particularly relevant to esthetic restorative procedures, in which changes in the optical properties of the underlying dentin may influence the final restorative outcome. Therefore, identifying natural biomodifying agents capable of improving collagen properties without compromising dentin color remains relevant.

Rutin (vitamin P) is a plant-derived glycosylated flavonoid with antioxidant and anti-inflammatory properties [10, 11]. Although rutin has been less extensively investigated in dentin than other natural biomodifiers, previous evidence provides a biological rationale for investigating it as a potential collagen biomodifying agent. Studies involving collagen-containing tissues and collagen-related structures have reported effects associated with rutin and suggested that its molecular characteristics may favor interactions with collagen [12,13,14]. In addition, modulation of matrix metalloproteinase activity by rutin has been reported in non-dental biological models [12, 14, 15]. These findings provide a rationale for investigating rutin in dentin, although they do not establish its mechanism of action in dentin collagen.

Despite this biological rationale, the effects of rutin on dentin collagen remain largely unexplored. In particular, its potential interaction with dentin collagen and its influence on mechanical properties have not been clearly established. Furthermore, because color alterations have been associated with other natural biomodifying agents [5, 9, 15], the optical behavior of dentin after rutin application is also relevant, particularly for esthetic restorative procedures. However, the effect of topical rutin application on dentin collagen color has not been established. Evaluating both mechanical behavior and color changes may therefore provide a more comprehensive initial assessment of rutin as a potential dentin biomodifying agent.

Therefore, the aim of this study was to evaluate the biomodifying effect of rutin extracted from Dimorphandra gardneriana on the tensile strength and color change of dentin collagen. The null hypotheses were that: (1) no significant differences would be detected in the tensile strength of dentin collagen among the groups; and (2) rutin concentration and biomodification time would not significantly affect dentin collagen color.

Materials and methods

Rutin extraction

One hundred and fifty grams of Dimorphandra gardneriana seeds were subjected to Soxhlet extraction using hexane, ethyl acetate, methanol, and water as solvents. The resulting extracts were concentrated using a rotary evaporator. After thin-layer chromatography (TLC) analysis, the ethyl acetate and methanolic extracts were combined and dispersed in 200 mL of cold water. The mixture was agitated and filtered, and the resulting residue was washed with an additional 100 mL of water. After filtration, the residue was dried in an oven at 100 °C. The dried material was then subjected to silica gel column chromatography and eluted with mixtures of hexane, dichloromethane, ethyl acetate, and methanol of increasing polarity. Fractions were collected and compared by TLC, resulting in the purification of rutin.

Preparation of the aqueous rutin solutions

The rutin concentrations were selected a priori based on the limited aqueous solubility of rutin. The highest concentration (0.0125% w/v) corresponded to the reported water solubility of rutin (0.125 g/L) [17], whereas 0.008% and 0.004% (w/v) were selected as progressively lower concentrations to investigate its biomodifying effect within this aqueous concentration range.

Rutin was weighed using an analytical balance (AUX-220, Shimadzu, Tokyo, Japan) and dissolved in distilled water (pH = 7.01) using a vortex mixer (QL-901, Biomixer, São Paulo, SP, Brazil) to obtain aqueous rutin solutions at concentrations of 0.004% (pH = 6.72), 0.008% (pH = 6.40), and 0.0125% (pH = 6.22) (w/v). The pH of each solution was measured immediately after preparation using a digital pH meter (QUIMIS, model Q400AS, Diadema, SP, Brazil).

Specimen preparation and experimental design

A total of 244 sound, unerupted human third molars were used in this study after informed consent was obtained under a protocol reviewed and approved by the local Research Ethics Committee (approval no. 2.006.679). The teeth were stored in 0.1% thymol solution and used within 1 month after extraction. Two independent experiments were conducted to evaluate the effects of rutin on the tensile strength and color of demineralized dentin collagen.

Experiment 1—Tensile strength

Forty teeth were used to prepare the specimens for tensile strength testing. Dentin discs (1.7 ± 0.1 mm thick) were obtained from the mid-coronal portion of each tooth using a diamond blade (Extec model 12205; Extec Corp., Enfield, CT, USA) mounted on a metallographic cutting machine (Isomet; Buehler, Lake Bluff, IL, USA) under copious water cooling. Each dentin disc was sectioned to produce rectangular dentin specimens measuring approximately 0.5 mm in thickness × 1.7 mm in width × 6.0 mm in length. A total of 120 rectangular specimens were obtained and randomly allocated (Excel 2019; Microsoft Corp., Redmond, WA, USA) to 12 experimental groups (n = 10). Specimens obtained from the same tooth were distributed among different experimental groups. Each specimen was considered an independent experimental unit for statistical analysis.

Experiment 2—Color change

Two hundred and four additional teeth were used for quantitative color analysis. One mid-coronal dentin disc (1.7 ± 0.1 mm thick) was obtained from each tooth using the same procedure described above, resulting in 204 independent specimens. The specimens were randomly allocated to 12 experimental groups (n = 17).

For both experiments, the experimental design consisted of four treatments—distilled water (control) and aqueous rutin solutions at concentrations of 0.004%, 0.008%, and 0.0125%—combined with three application times (1, 30, and 60 min), resulting in 12 experimental groups (Table 1).

Table 1 Experimental design.

Full size table

Sample size and power analyses

For Experiment 1 (tensile strength), an a priori sample size calculation had not been performed. Therefore, a sensitivity analysis was conducted using G*Power to estimate the minimum detectable effect size for the available sample size. Considering N = 120, α = 0.05, statistical power of 80%, and 3 numerator degrees of freedom for the main treatment effect, the minimum detectable effect size was f = 0.307.

For Experiment 2 (color change), ΔEab was defined as the primary color outcome. The sample size was planned using preliminary data from the initial quantitative color assessment, from which an effect size of f = 0.239 was estimated for the main treatment effect. An a priori power analysis was performed using GPower (version 3.1; Heinrich Heine University Düsseldorf, Düsseldorf, Germany), considering a factorial design with four treatment levels and three application times, a significance level of α = 0.05, statistical power of 80%, and 3 numerator degrees of freedom for the main treatment effect. The analysis indicated a minimum total sample size of 196 specimens. To maintain equal allocation among the 12 experimental groups, the sample size was increased to 204 specimens, corresponding to 17 specimens per group.

Dentin collagen biomodification

The dentin biomodification protocol was performed according to Bedran-Russo et al. [8] (Fig. 1). In both experiments, the specimens were completely demineralized in 10% phosphoric acid (Ethical Laboratory, Fortaleza, CE, Brazil) for 5 h. The specimens were then immersed in 1.5 mL of their respective biomodifying solution—distilled water (control) or aqueous rutin solution at concentrations of 0.004%, 0.008%, or 0.0125%—for 1, 30, or 60 min, according to their experimental group. After biomodification, the specimens were rinsed with distilled water for 1 min and blot-dried.

Fig. 1: Schematic representation of the experimental design.

Two independent experimental sets were established for tensile strength and quantitative color analysis. After specimen preparation and dentin demineralization, specimens were biomodified with distilled water (control) or aqueous rutin solutions (0.004%, 0.008%, or 0.0125%) for 1, 30, or 60 min. Tensile strength was evaluated using a universal testing machine, whereas color stability was assessed spectrophotometrically before and after biomodification.

For Experiment 2, baseline color measurements were performed after complete demineralization and immediately before biomodification, as described below.

Tensile strength testing

For Experiment 1, following dentin collagen biomodification, each rectangular collagen specimen was fixed with a cyanoacrylate-based adhesive (Super Bonder Gel, Loctite, São Paulo, SP, Brazil) in a modified Geraldeli device. The device was mounted in a universal testing machine (EMIC 23-10; Instron Inc., Canton, MA, USA), and tensile loading was applied at a crosshead speed of 1 mm/min until specimen failure. The load at failure was recorded and used to calculate collagen tensile strength (MPa).

Dentin collagen color evaluation

For Experiment 2, the baseline color of each demineralized collagen specimen was measured immediately before biomodification using a spectrophotometer (VITA Easyshade® Advance 4.0, Vident, Brea, CA, USA). Following biomodification, a second color measurement was performed using the same spectrophotometer under standardized conditions. Color measurements were recorded according to the CIE Lab* color space, in which L* represents lightness, a* represents the red–green axis, and b* represents the yellow–blue axis. Changes in each color coordinate between baseline and post-biomodification measurements were expressed as ΔL*, Δa*, and Δb*.

The overall color difference (ΔE*ab) between baseline and post-biomodification measurements was calculated using the following equation:

$$\Delta {{{\rm{Eab}}}}={[{(\Delta {{{\rm{L}}}})}^{2}+{(\Delta {{{{\rm{a}}}}}^{* })}^{2}+{(\Delta {{{{\rm{b}}}}}^{* })}^{2}]}^{1/2}$$

All spectrophotometric measurements were standardized with respect to specimen positioning, ambient lighting, temperature, and humidity. The measuring aperture was positioned perpendicular to the collagen surface at the same location for baseline and post-biomodification measurements.

Statistical analysis

Statistical analyses were performed using SigmaStat 4.0 (Systat Software Inc., San Jose, CA, USA). The Shapiro–Wilk test was used to assess normality, and the Brown–Forsythe test was used to assess homogeneity of variances. Tensile strength and quantitative color outcomes (ΔL*, Δa*, Δb*, and ΔE*ab) were analyzed separately using two-way ANOVA, with treatment and application time as factors. When significant effects were detected, the Student–Newman–Keuls test was used for post hoc group comparisons. The significance level was set at α = 0.05. For both experiments, each specimen was considered an independent experimental unit.

Ethics approval and consent to participate

Approved by the local Research Ethics Committee (protocol no. 2.006.679). Written informed consent was obtained from all donors.

Results

Experiment 1—Tensile strength testing

Tensile strength results are presented in Table 2. Two-way ANOVA revealed a significant effect of treatment (F = 30.342, p < 0.001), whereas neither biomodification time (F = 0.045, p = 0.956) nor the treatment × time interaction (F = 0.584, p = 0.743) was significant. Rutin-treated specimens showed significantly higher tensile strength than the control specimens (p < 0.05), whereas no significant differences were detected among the three rutin concentrations (p > 0.05).

Table 2 Dentin collagen tensile strength (MPa, mean ± SD) according to treatment and time.

Full size table

Experiment 2—Dentin collagen color evaluation

The results for ΔL*, Δa*, Δb*, and ΔE*ab are presented in Table 3. Two-way ANOVA revealed no significant effects of treatment, biomodification time, or treatment × biomodification time interaction on any of the evaluated color parameters (p > 0.05).

Table 3 Mean values of color coordinates (ΔL, Δa, Δb and ΔE) of dentin after rutin biomodification.

Full size table

No significant effects of treatment were observed for ΔL* (F = 0.106, p = 0.957), Δa* (F = 1.256, p = 0.291), Δb* (F = 1.950, p = 0.123), or ΔEab (F = 1.624, p = 0.185). Similarly, biomodification time had no significant effect on ΔL (F = 0.247, p = 0.782), Δa* (F = 0.248, p = 0.780), Δb* (F = 0.628, p = 0.535), or ΔEab (F = 0.955, p = 0.387). No significant treatment × biomodification time interactions were observed for ΔL (F = 1.048, p = 0.396), Δa* (F = 0.315, p = 0.929), Δb* (F = 0.636, p = 0.702), or ΔE*ab (F = 0.396, p = 0.881).

Discussion

The present study showed that rutin extracted from Dimorphandra gardneriana significantly increased the tensile strength of demineralized dentin collagen compared with the control treatment. No significant differences were detected among the rutin concentrations or application times evaluated. Regarding color, quantitative spectrophotometric analysis revealed no statistically significant effects of treatment, application time, or their interaction on the evaluated color parameters. Overall, these findings indicate that rutin increased the tensile strength of demineralized dentin collagen under the experimental conditions tested, whereas no treatment-related differences in color variation were detected. Therefore, the first null hypothesis was rejected, as rutin treatment increased the tensile strength of demineralized dentin collagen compared with the control. In contrast, the results failed to reject the second null hypothesis, as rutin concentration and biomodification time did not significantly affect dentin collagen color.

Evidence specifically addressing the effects of rutin on dentin collagen is scarce. Choi et al. [12] reported that topical rutin application increased the elastic modulus of human skin, while Plonska-Brzezinska et al. [13] described interactions between rutin and collagen-related structures. Although these findings provide biological plausibility for an interaction between rutin and collagen, they were obtained from experimental models distinct from dentin and therefore cannot directly explain the increased tensile strength observed in the present study. Nevertheless, the higher tensile strength of rutin-treated specimens compared with the control indicates that exposure to rutin affected the mechanical behavior of the demineralized dentin collagen matrix.

The molecular mechanisms underlying this effect remain uncertain. Previous studies have suggested that the hydroxyl groups of rutin may participate in hydrogen bonding, whereas its aromatic structures may contribute to hydrophobic interactions with collagen-related structures [13]. Rutin has also been associated with modulation of matrix metalloproteinase activity in non-dental biological models [11, 14, 15]. Such mechanisms are relevant because collagen stabilization and reduced enzymatic degradation have been proposed for other natural biomodifying agents. However, the present study did not directly assess rutin–collagen interactions, collagen cross-linking, or MMP inhibition. Therefore, the increase in tensile strength observed here cannot be attributed to any specific molecular mechanism. Spectroscopic, microscopic, and biochemical analyses will be necessary to determine whether these proposed interactions occur in dentin collagen.

EGCG provides a useful reference for contextualizing these findings because it is a flavonoid-derived compound that has been more extensively investigated as a dentin biomodifier. Previous studies have demonstrated interactions between EGCG and collagen and inhibition of collagen degradation [7], providing more direct evidence of its effects on the dentin collagen matrix. In contrast, evidence supporting rutin as a dentin biomodifier remains limited, and the present study primarily provides evidence of a mechanical effect rather than the molecular mechanism responsible for it. Thus, similarities in the biological properties attributed to EGCG and rutin should not be interpreted as evidence that they act through the same mechanisms or have comparable effectiveness. Direct comparative studies would be necessary to determine whether rutin offers mechanical, chemical, or optical advantages over established natural biomodifiers such as EGCG.

No statistically significant differences were detected among the rutin concentrations evaluated (0.004%, 0.008%, and 0.0125%). This finding does not establish equivalence among concentrations or confirm the presence of a plateau in the biomodifying effect of rutin. Although plateau effects have been reported for other natural collagen cross-linking agents [1, 5], the dose–response behavior of rutin in dentin collagen remains unclear. The relatively narrow concentration range investigated may have limited the characterization of a concentration-dependent response. In addition, the concentration range was constrained by the limited aqueous solubility of rutin, as higher concentrations may require alternative solvents or solubilization strategies. Therefore, the highest concentration evaluated (0.0125%) should not be regarded as an optimal biological concentration, but rather as the upper concentration investigated within the physicochemical constraints of the aqueous experimental system used in this study. Furthermore, the sensitivity analysis indicated that the experimental design had 80% power to detect treatment effects of f = 0.307 or greater; thus, smaller differences among concentrations may have remained undetected. Further studies using a broader concentration range and specifically designed to characterize the dose–response relationship of rutin are warranted.

Application time did not significantly affect tensile strength, and no significant treatment × time interaction was observed. The 30- and 60-min application periods were included as experimental conditions to determine whether prolonged exposure to rutin would produce a time-dependent effect on dentin collagen, as extended application times have commonly been used in laboratory studies of dentin biomodification with natural agents [1, 8, 17]. However, such prolonged application times have limited clinical feasibility. Therefore, a 1-min application period was also included to investigate the response to a shorter exposure that could be more compatible with a future dentin pretreatment protocol. The absence of a statistically significant time effect indicates that, within the conditions and sensitivity of the present experiment, prolonged exposure did not produce a detectable additional increase in tensile strength. Nevertheless, these findings do not demonstrate that a 1-min application is clinically sufficient or optimal.

Color represents an additional consideration when natural compounds are proposed as dentin biomodifiers, particularly because some agents may alter the optical characteristics of the substrate. PA-based agents, for example, have been associated with dentin discoloration [1, 8, 16, 18], while color alterations have also been reported in studies involving EGCG-containing approaches [9]. In the present study, quantitative spectrophotometric evaluation showed no statistically significant effects of rutin treatment, application time, or their interaction on color variation. Under the conditions evaluated, the tested rutin treatments therefore did not produce statistically detectable color differences compared with the control. Nevertheless, the absence of statistically significant differences does not establish equivalence among treatments or demonstrate that rutin produces no color change. Furthermore, because color was evaluated immediately after biomodification, the present results do not establish long-term color stability.

Taken together, the mechanical and color findings provide an initial basis for investigating rutin as a potential dentin biomodifying agent. However, they do not demonstrate that rutin is superior to other natural biomodifiers such as EGCG or PAs. Likewise, the lack of statistically detectable treatment-related color differences in the present experiment should not be considered evidence of a clinical esthetic advantage. Direct comparisons with established biomodifiers, together with long-term mechanical and spectrophotometric evaluations, are required to determine whether rutin presents any relevant advantages for restorative applications.

The in vitro nature of the present study should be considered when interpreting these findings. The use of fully demineralized dentin allowed the collagen matrix to be evaluated under controlled conditions but does not reproduce the more complex substrate encountered during adhesive restorative procedures. The experimental conditions also did not simulate relevant challenges of the oral environment, including pH fluctuations, thermal cycling, and enzymatic degradation, and no bonding protocol was performed. Because dentin biomodification is particularly relevant to the long-term stability of the collagen matrix, the immediate increase in tensile strength observed in the present study does not establish the durability of the biomodifying effect. Previous studies with other naturally derived collagen cross-linkers have demonstrated that the effects of dentin biomodification on resin–dentin bonding may persist during long-term storage, although these effects depend on the biomodifying agent and adhesive system [19, 20]. Therefore, aging studies are necessary to determine whether the mechanical effect observed after rutin treatment is maintained over time. The present findings should thus be regarded as laboratory evidence of the potential effect of rutin on demineralized dentin collagen rather than evidence of clinical effectiveness.

Conclusions

Within the limitations of this in vitro study, rutin extracted from Dimorphandra gardneriana increased the immediate tensile strength of demineralized dentin collagen compared with the control. No significant differences were observed among rutin concentrations or application times, and no treatment-related differences in color variation were detected under the conditions evaluated.

Data availability

Data are available from the corresponding author on reasonable request.

References

  1. Bedran-Russo AK, Pauli GF, Chen SN, McAlpine J, Castellan CS, Phansalkar RS, et al. Dentin biomodification: strategies, renewable resources and clinical applications. Dent Mater. 2010;30:62–76. https://doi.org/10.1016/j.dental.2013.10.012.

  2. Braga GPA, Caiaffa KS, Rabelo RL, Santos VRD, Souza ACA, Ribeiro LDS, et al. Cytotoxicity and biomineralization potential of flavonoids incorporated into PNVCL hydrogels. J Funct Biomater. 2023;14:139. https://doi.org/10.3390/jfb14030139.

  3. Fang M, Liu R, Xiao Y, Li F, Wang D, Hou R, et al. Biomodification to dentin by a natural crosslinker improved the resin-dentin bonds. J Dent. 2012;40:458–66. https://doi.org/10.1016/j.dental.2013.07.015.

  4. Breschi L, Maravic T, Cunha SR, Comba A, Cadenaro M, Tjäderhane L, et al. Dentin bonding systems: from dentin collagen structure to bond preservation and clinical applications. Dent Mater. 2018;34:78–96. https://doi.org/10.1016/j.dental.2017.11.005.

  5. Dávila-Sánchez A, Gutierrez MF, Bermudez JP, Méndez-Bauer ML, Hilgemberg B, Sauro S, et al. Influence of flavonoids on long-term bonding stability on caries-affected dentin. Dent Mater. 2020;36:1151–60. https://doi.org/10.1016/j.dental.2020.05.007.

  6. Hiraishi N, Sono R, Sofiqul I, Yiu C, Nakamura H, Otsuki M, et al. In vitro evaluation of plant-derived agents to preserve dentin collagen. Dent Mater. 2013;29:1048–54. https://doi.org/10.1016/j.dental.2013.07.015.

    Article  CAS  PubMed  Google Scholar 

  7. Jackson JK, Zhao J, Wong W, Burt HM. The inhibition of collagenase induced degradation of collagen by the galloyl-containing polyphenols tannic acid, epigallocatechin gallate and epicatechin gallate. J Mater Sci Mater Med. 2010;21:1435–43. https://doi.org/10.1007/s10856-010-4019-3.

  8. Bedran-Russo AK, Pereira PN, Duarte WR, Drummond JL, Yamauchi M. Application of crosslinkers to dentin collagen enhances the ultimate tensile strength. J Biomed Mater Res Part B Appl Biomater. 2007;80:268–72. https://doi.org/10.1002/jbm.b.30593.

  9. Lopes RG, Oliveira-Reis B, Maluly-Proni AT, Silva MHT, Briso ALF, dos Santos PH. Influence of green tea extract in the color of composite resin restorations. J Mech Behav Biomed Mater. 2019;100:103408. https://doi.org/10.1016/j.jmbbm.2019.103408.

  10. Sharma A, Tirpude NV, Bhardwaj N, Kumar D, Padwad Y. Berberis lycium fruit extract and its phytoconstituents berberine and rutin mitigate collagen-CFA-induced arthritis (CIA) via improving GSK3β/STAT/Akt/MAPKs/NF-κB signaling axis mediated oxi-inflammation and joint articular damage in murine model. Inflammopharmacology. 2022;30:655–66. https://doi.org/10.1007/s10787-022-00941-z.

  11. Chen WY, Huang YC, Yang ML, Lee CY, Chen CJ, Yeh CH, et al. Protective effect of rutin on LPS-induced acute lung injury via down-regulation of MIP-2 expression and MMP-9 activation through inhibition of Akt phosphorylation. Int Immunopharmacol. 2014;22:409–13. https://doi.org/10.1016/j.intimp.2014.07.026.

  12. Choi SJ, Lee SN, Kim K, Joo da H, Shin S, Lee J, et al. Biological effects of rutin on skin aging. Int J Mol Med. 2016;38:357–63. https://doi.org/10.3892/ijmm.2016.2604.

  13. Plonska Brzezinska ME, Bobrowska DM, Sharma A, Rodziewicz P, Tomczyk M, Czyrko J, et al. Triple helical collagen like peptide interactions with selected polyphenolic compounds. RSC Adv. 2015;5:95443–53. https://doi.org/10.1039/c5ra15469c.

  14. Albaqami FF, Althurwi HN, Alharthy KM, Hamad AM, Awartani FA. Rutin gel with bone graft accelerates bone formation in a rabbit model by inhibiting MMPs and enhancing collagen activities. Pharmaceuticals. 2023;16:774. https://doi.org/10.3390/ph16050774.

  15. Selvaraj G, Kaliamurthi S, Thiruganasambandam R. Molecular docking studies of rutin on matrix metalloproteinase. Insight Biomed. 2016;1:1–5. https://doi.org/10.1515/jbcpp-2020-0036.

  16. Enrich-Essvein T, González-López S, Rodríguez-Navarro AB, Cifuentes-Jiménez C, Maravic T, Mazzitelli C, et al. Effects of proanthocyanidin-functionalized hydroxyapatite nanoparticles on dentin bonding. Clin Oral Investig. 2024;28:444 Jul 24. https://doi.org/10.1007/s00784-024-05836-7.

  17. Pedriali CA, Fernandes AU, Bernusso LC, Polakiewicz B. The synthesis of a water-soluble derivative of rutin as an antiradical agent. Quim Nova. 2008;31:2147–51. https://doi.org/10.1590/S0100-40422008000800039.

  18. Hechler B, Yao X, Wang Y. Proanthocyanidins alter adhesive/dentin bonding strengths when included in a bonding system. Am J Dent. 2012;25:276–80. Oct.

    PubMed  PubMed Central  Google Scholar 

  19. Castellan CS, Bedran-Russo AK, Antunes A, Pereira PNR. Effect of dentin biomodification using naturally derived collagen cross-linkers: one-year bond strength study. Int J Dent. 2013;2013:918010. https://doi.org/10.1155/2013/918010.

  20. Hardan L, Daood U, Bourgi R, Cuevas-Suárez CE, Devoto W, Zarow M, et al. Effect of collagen crosslinkers on dentin bond strength of adhesive systems: a systematic review and meta-analysis. Cells. 2022;11:2417. https://doi.org/10.3390/cells11152417.

Download references

Acknowledgements

The authors thank the donors and the participating institutions for technical support.

Funding

This research was supported by the Fundação Cearense de Apoio ao Desenvolvimento Científico e Tecnológico (FUNCAP), under grant number BMD-0008-01278.01.08/23.

Author information

Authors and Affiliations

  1. Master in Dental Sciences, University Christus (UNICHRISTUS), Fortaleza, Brazil

    Lara R. Aragão, Paulo G. B. Silva & Jiovanne R. Neri

  2. School of Dentistry, University Christus Christus (UNICHRISTUS), Fortaleza, Brazil

    Isabely B. Freitas

  3. Graduate Program in Biotechnology, Universidade Estadual do Ceará (UECE), Fortaleza, Brazil

    Selene M. de Morais, Solange de O. Pinheiro, Ícaro G. P. Vieira & Wildson M. B. da Silva

  4. School of Dentistry, Universidade de Fortaleza (UNIFOR), Fortaleza, Brazil

    Marcelo V. S. Lemos

  5. Department of Restorative Dentistry, Faculty of Pharmacy, Dentistry and Nursing, Universidade Federal do Ceará (UFC), Fortaleza, Brazil

    Sérgio L. Santiago

Authors

  1. Lara R. Aragão
  2. Isabely B. Freitas
  3. Selene M. de Morais
  4. Solange de O. Pinheiro
  5. Ícaro G. P. Vieira
  6. Wildson M. B. da Silva
  7. Paulo G. B. Silva
  8. Marcelo V. S. Lemos
  9. Sérgio L. Santiago
  10. Jiovanne R. Neri

Contributions

Conceptualization: JRN, SLS; Methodology: LRA, IBF, IRSL, WMBS, PGBS; Rutin extraction/purification: SMM, SOP, ÍGPV; Investigation: LRA, IBF, IRSL; Formal analysis: LRA, IBF, PGBS, Supervision: MVSL, SLS, JRN; Writing—original draft: LRA, JRN; Writing—review and editing: all authors.

Corresponding author

Correspondence to Jiovanne R. Neri.

Ethics declarations

Competing interests

The authors declare no competing interests.

Additional information

Publisher’s note Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Rights and permissions

Open Access This article is licensed under a Creative Commons Attribution 4.0 International License, which permits use, sharing, adaptation, distribution and reproduction in any medium or format, as long as you give appropriate credit to the original author(s) and the source, provide a link to the Creative Commons licence, and indicate if changes were made. The images or other third party material in this article are included in the article’s Creative Commons licence, unless indicated otherwise in a credit line to the material. If material is not included in the article’s Creative Commons licence and your intended use is not permitted by statutory regulation or exceeds the permitted use, you will need to obtain permission directly from the copyright holder. To view a copy of this licence, visit http://creativecommons.org/licenses/by/4.0/.

Reprints and permissions

About this article

Check for updates. Verify currency and authenticity via CrossMark

Cite this article

Aragão, L.R., Freitas, I.B., de Morais, S.M. et al. Biomodifying effect of rutin extracted from Dimorphandra gardneriana on tensile strength and color change of dentin collagen. BDJ Open 12, 115 (2026). https://doi.org/10.1038/s41405-026-00506-0

Download citation

  • Received: 19 February 2026

  • Revised: 17 September 2026

  • Accepted: 01 October 2026

  • Published: 18 November 2026

  • Version of record: 18 November 2026

  • DOI: https://doi.org/10.1038/s41405-026-00506-0

来源:Nature 健康护理主题 · nature.com